Inconel 625 Sheet & Coil

Nickel-Base Superalloy

Inconel 625 (UNS Designation N06625)

Physical Properties

Thermal Conductivity
Temperature Range Linear Coefficients of Thermal Expansion1 · 10-6 Thermal Conductivity2 3
°C °F /°C /°F W/m·K Btu/(hr/ft²/in/°F)
-157-250--7.34.2
-129-200--7.44.3
-73-100--8.34.8
-180--9.25.3
2170--9.95.7
38100--10.05.8
9320012.87.110.76.3
20440013.17.312.67.3
31660013.37.414.28.2
42780013.77.615.79.1
538100014.07.817.510.1
649120014.88.219.011.0
760140015.38.520.812.0
871160015.88.822.813.2
927170016.29.0--
9821800--25.314.6
  1. Average coefficient from 70°F (21°C) to temperature shown
  2. Measurements made at Battelle Memorial Institute
  3. Material annealed 2100°F (1149°C)
Electrical Resistivity
Temperature microhm-cm
°C °F
2170128.9
38100129.6
93200131.9
204400133.9
316600134.9
427800135.9
5381000137.9
6491200137.9
7601400136.9
8711600135.9
9821800134.9
10932000133.9